What does type of fracture tell us about the cylinder test result? |
| |
|
|
Q. Is there any information on the significance of different types of breaks when cylinders are tested for compressive strength? I'm particularly interested in what are considered "good" break types versus "bad" break types. For instance, if the strength is lower than expected, can the break type help to indicate whether the low strength was caused by a testing problem rather than a problem with the concrete?
A. Figure 1, from ASTM C 39-03, "Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens," shows five different types of fracture. This standard requires that reports include the type of fracture "if other than the usual cone."

A cone failure results when friction at the platens of the testing machine restrains lateral expansion of the concrete as the vertical compressive force is applied. This restraint confines the concrete near the platens and results in two relatively undamaged cones when the cylinder is tested to fracture. If the friction were eliminated, the cylinder would expand more laterally and exhibit a splitting failure similar to that shown in Fig. l(e). Such vertical splitting has been observed in numerous tests on high-strength specimens made of mortar or neat cement paste, but the effect is less common in ordinary concrete when coarse aggregate is present (Neville, A., Properties of Concrete, 4th Ed., Prentice Hall, 1995).
The "Manual of Aggregate and Concrete Testing," included as related material in Volume 4.02 of the 2003 Annual Book of ASTM Standards, states that the type of fracture may be of assistance in determining the cause for the compressive strength of a tested cylinder being less than anticipated. The manual describes a case in which a fracture type that didn't match any of those in Fig. 1 had been noted in a large number of tested cylinders. A photo of the atypical failure shows a crack parallel to the ends and at about midheight in the cylinder. This failure mode was taken as an indicator of nonstandard testing procedures. The ASTM documents don't give any further information regarding causes for types of fracture other than the typical cone or whether any of the types shown are bad or good.
When unbonded neoprene caps are used to determine concrete compressive strength, the broken cylinder only rarely exhibits the conical fracture typical of capped cylinders, and the sketches shown in Fig. 1 aren't descriptive (ASTM C 1231, "Standard Practice for Use of Unbonded Caps in Determination of Compressive Strength of Hardened Concrete Cylinders"). When neoprene caps are used, if requirements for perpendicularity of the cylinder ends or vertical alignment during loading aren't met, load applied to the cylinder may be concentrated on one side of the specimen. This can cause a short shear failure similar to that shown in Fig. l(d), except that the failure plane intersects the end of the cylinder. This type of fracture generally indicates the cylinder failed prematurely, yielding results lower than the actual strength of the concrete (Kosmatka, Kerkhoff, and Panarese, “Design and Control of Concrete Mixtures,” PCA, 2002).
We could find no other reports or textbooks that related fracture type to testing variables or concrete properties.
---------- To purchase ASTM standards referenced above, visit the website: http://www.astm.org
To purchase PCA documents referenced above, visit the bookstore at: http://www.cement.org/bookstore/
To purchase the book by Neville, visit websites such as http://www.amazon.com
Purchase ACI documents at the ACI Bookstore
Posted 2/13/06.
Disclaimer: Questions in this column were asked by users of ACI documents and have been answered by ACI staff or by a member or members of ACI technical committees. The answers do not represent the official position of an ACI committee. Only a published committee document represents the formal consensus of the committee and the Institute.
|
|
| |
Was this answer useful?
 |
|
 |
|